美女一级片在线观看_天天狠天天射日韩三级黄视频_五月丁香色色婷婷_成人无码视频免费看_日韩免费黄色在线视频_国产精品无码视屏_日本无码中字caobi在线_亚洲福利盛宴在线观看

Welcome to Changzhou bidafu plastic profile co., ltd! Main products: PC tube, PC lampshade, acrylic lampshade, etc
Changzhou bidafu plastic profile co., ltd

Professional Production of PC Tubes, Acrylic

Hotline0519-86393611
Popular Keywords:

News

Contact Us
Hotline:0519-86393611
Address:Hutang Town, Changzhou City, Jiangsu Province
Tel:0519-86393611
Fax:0519-89612639
Email:fuermaxc@126.com
Post Encoding:
Technology
jishuzhichi
Causes and Solutions of Profile Groove

Profiles will have dents in the production process, so what is the reason for the dents? What is the solution?

Causes of dents: different thickness of parts of products, insufficient internal pressure of dies, insufficient cooling of dies, and deformation due to insufficient cooling time

Associated knowledge

In the process of producing products, dents are the most frequent adverse phenomena. When the plastic injected into the mould is cooled, volume shrinkage occurs. The early cooling part, i.e. the surface hardens first, and bubbles will appear inside. The so-called dent is that the slow cooling part produces conspicuous concave surface in the direction of bubble shrinkage.

Large shrinkage materials are also prone to dents. When changing the forming conditions to eliminate dents, the setting conditions should be set in the direction of small shrinkage. That is, the die temperature and the barrel temperature decrease, and the injection pressure increases, but it should be noted that the residual internal stress may be caused by this.

Because the indentation is better not to be conspicuous, if it does not affect the appearance, it is intentionally processed into corrosion patterns on the die, such as grain, granular and so on. Also, if the forming material is HIPS, reducing the mold temperature to reduce the smoothness is also effective. But once these methods have dents, it is difficult to repair polished products.

Resolvent

Instant: Increase injection pressure, prolong injection holding time, reduce barrel temperature and die temperature, and force cooling in the place where dents occur.

Short-term: Fill in the runner where the dent occurs (Fig. A). When there is a narrow area along the edge of the material where the dent occurs, the edge is thicker (Fig. B).

Long-term: The thickness difference of design products should be completely avoided. Reinforcement tendons prone to dents should be as short as possible in narrow and long shapes (Fig. C).

Material differences

The material with large shrinkage in moulding also has large dents.

For example, PE, PP, even if only slightly reinforced, will produce dents.

Molding shrinkage of materials PS0.002~0.006PP0.01~0.02PE0.02~0.05

Matters needing attention

When the temperature decreases to zero, if there is pressure on the material in the die cavity, it should be considered that no dent will occur. The pressure of the material surrounding the die, i.e. the static pressure, is not necessarily anywhere in the die.

If the pressure near the gate is high, if the material passes wide, because of the pressure transfer to each corner, the pressure difference between the near gate and the place far from the gate is very small compared with the whole pressure, there will be no dent, and the products without residual internal stress will be obtained.

When part of the material flows into a difficult place, there is high pressure in this place, and when the pressure in other places decreases, there will be dents. This part of the high pressure residue is the internal stress of the product is also large. In the ideal state, the material fluidity is better when the temperature of the material rises with the temperature of the die, and the ejection also changes to the bottom in the static pressure state.

When changing the forming conditions, the combination of temperature, pressure and time should be prepared in advance, and the results can be known in order. After a long time, it's easy to know when the pressure changes slightly. It should be noted that when the temperature changes, the results should be obtained after injection material, and when the temperature drops, the results should be reproduced.


Return To The Top
主站蜘蛛池模板: 日韩与欧美特级毛片合作作品| 黄网站在线观看免费不卡无码| 一级二级毛片亚洲乱伦蜜桃| 三级av在线日韩精品爆菊花| 欧美成人性生活片在钱| 我想看日韩的黄片| 99色色这里有精品| 久久六月无码一区| 国产在线伊人日逼黄片| 少妇一二三区免费中文字幕视频| 人妻少妇中文字幕| 自拍亚洲无码密臀综合久久| 青青草一区二区免费精品| 超碰揉揉人人操人人摸| 亚洲黄片观看亚洲国产黑丝| 亚洲女成人综合亚洲免费视| 免费在线有码视频| 亚洲激情成人网| 国产精品不卡精品综合在| 波多野结衣二区| 欧美日韩嫖妓成人激情开心| WWW在线а日韩婷婷| 98精品国产一区二区三区入口| 激情五月日本不卡| 日韩成人小电影| 国产成人精品一区二三区在线| 免费国产一级午夜导航福利| 区一区二性网站| 久久人妻丝袜中久草娱乐| 免费成人网站在线| 黄色一区二区三区在线观看| 成人毛片激情免费播放| 日韩成人免费视频看看| 天天操夜夜操草草草视频在线| 成人婷婷五月天| www人人人操10区av| 特级一内黄片丰满美女的A片| 欧美人妻性爱精品| 射丝袜视频色香操AV亚洲 | 亚州午夜毛片色色中文字幕| 国产成人综合av|